QA/QC  › Testing Lab  › Field Slump Test
Test-report · QC-TLB-TST-001
Field Slump Test Record
16 checkpoints across 6 sections. Every concrete batch before placement; retest if delay > 30 min from batching
16 Checkpoints
6 Sections
Per batch / per transit mixer
Site QC Engineer, Lab Technician

Checklist Preview

S.No.CheckpointIS RequirementStatus
A. APPARATUS AND SAMPLING
A1Slump cone per IS 1199 Part 2: 200 mm bottom × 100 mm top × 300 mm height; internally clean and damp
Acceptance: Cone dimensions within tolerance; handles and foot-pieces intact; wiped clean before test
Cl. 4 — Apparatus
OK
NC
NA
HOLD
A2Tamping rod 16 mm dia × 600 mm long with rounded end used
Acceptance: Steel rod with hemispherical end; dimensions per IS
Cl. 4 — Tamping rod
OK
NC
NA
HOLD
A3Sample collected from 3 or more portions of the batch at point of discharge
Acceptance: Representative sample ≥ 0.03 cu.m; collected within 15 minutes after discharge
Cl. 6 — Sampling
OK
NC
NA
HOLD
B. TEST PROCEDURE
B1Cone placed on smooth, level, non-absorbent surface; held down by operator's feet
Acceptance: Base plate flat; cone held firm; no movement during filling
Cl. 7 — Placement
OK
NC
NA
HOLD
B2Concrete filled in 3 layers, each ~1/3 volume, tamped 25 strokes per layer
Acceptance: 25 blows per layer; blows distributed uniformly; penetrate just into previous layer
Cl. 7 — Filling & tamping
OK
NC
NA
HOLD
B3Top surface struck off flush with top of cone using tamping rod
Acceptance: Excess removed; surface smooth and level with cone top
Cl. 7 — Finishing
OK
NC
NA
HOLD
B4Cone lifted vertically in 5-10 seconds without lateral or rotational motion
Acceptance: Vertical lift within 5-10 s; total test time from start of filling to cone removal ≤ 150 s
Cl. 7 — Cone removal
OK
NC
NA
HOLD
B5Slump measured as vertical distance between original top (cone height 300 mm) and displaced top
Acceptance: Measured at highest point using rod and steel rule; record to nearest 5 mm
Cl. 7 — Measurement
OK
NC
NA
HOLD
C. TEST READINGS
C1Record slump value (mm) — true slump; note if shear or collapse occurs, repeat test
Acceptance: True slump recorded; shear/collapse → invalid result, test repeated with fresh sample
Cl. 8 — Reporting
OK
NC
NA
HOLD
C2Observe cohesion and bleeding of slumped sample; note any segregation
Acceptance: Cohesive, no segregation, minimal bleeding; if excessive → mix re-design review
Cl. 8 — Visual assessment
OK
NC
NA
HOLD
Showing 10 of 16 checkpoints ·
A. APPARATUS AND SAMPLING
A1Slump cone per IS 1199 Part 2: 200 mm bottom × 100 mm top × 300 mm height; internally clean and damp
Cl. 4 — Apparatus (IS 1199)
Cone dimensions within tolerance; handles and foot-pieces intact; wiped clean before test
OKNCNAHOLD
A2Tamping rod 16 mm dia × 600 mm long with rounded end used
Cl. 4 — Tamping rod (IS 1199)
Steel rod with hemispherical end; dimensions per IS
OKNCNAHOLD
A3Sample collected from 3 or more portions of the batch at point of discharge
Cl. 6 — Sampling (IS 1199)
Representative sample ≥ 0.03 cu.m; collected within 15 minutes after discharge
OKNCNAHOLD
B. TEST PROCEDURE
B1Cone placed on smooth, level, non-absorbent surface; held down by operator's feet
Cl. 7 — Placement (IS 1199)
Base plate flat; cone held firm; no movement during filling
OKNCNAHOLD
B2Concrete filled in 3 layers, each ~1/3 volume, tamped 25 strokes per layer
Cl. 7 — Filling & tamping (IS 1199)
25 blows per layer; blows distributed uniformly; penetrate just into previous layer
OKNCNAHOLD
B3Top surface struck off flush with top of cone using tamping rod
Cl. 7 — Finishing (IS 1199)
Excess removed; surface smooth and level with cone top
OKNCNAHOLD
B4Cone lifted vertically in 5-10 seconds without lateral or rotational motion
Cl. 7 — Cone removal (IS 1199)
Vertical lift within 5-10 s; total test time from start of filling to cone removal ≤ 150 s
OKNCNAHOLD
B5Slump measured as vertical distance between original top (cone height 300 mm) and displaced top
Cl. 7 — Measurement (IS 1199)
Measured at highest point using rod and steel rule; record to nearest 5 mm
OKNCNAHOLD
C. TEST READINGS
C1Record slump value (mm) — true slump; note if shear or collapse occurs, repeat test
Cl. 8 — Reporting (IS 1199)
True slump recorded; shear/collapse → invalid result, test repeated with fresh sample
OKNCNAHOLD
C2Observe cohesion and bleeding of slumped sample; note any segregation
Cl. 8 — Visual assessment (IS 1199)
Cohesive, no segregation, minimal bleeding; if excessive → mix re-design review
OKNCNAHOLD
Showing 10 of 16 ·
Inspection Sign-Off
APPROVED
APPROVED WITH CONDITIONS
REJECTED — NCR RAISED
Remarks
Name / Sign / Date
Tested By
Name / Sign / Date
Reviewed / Approved By
Name / Sign / Date